Welding procedure specification for SMAW

Update ASME IX 2019
Deteled: QW-405.2

WPS for P-No. 1

P-1 Gr.-1

  • Material: API 5L X52 PSL1 Normalized ASME B36.10M SMLS
  • P-Number 1 and Gr-Number 1
  • Pipe size: NPS 8” Sch 80 (12.7 mm)
  • Joint design: Groove, included angle 60 deg.
  • Position: 6G
  • Welding process: SMAW deposit 12.7 mm, manual.

Recommend base metal is API 5L Gr. X52 PSL 1 SMLS

General

Description of WPS here.

Welding Variables

Paragraph Variables SMAW
QW-402 Joints
QW-402.1 change Groove design Groove
QW-402.4 delettion Backing With/Without backing
QW-402.10 change Root spacing 3.0 - 4.0 mm
QW-402.11 deletion/addition Retainers None
QW-403 Base Metals
QW-403.5 change Group Number Any Gr. 1 to any Gr. 1
QW-403.6 T limits toughness 12.7 to 25.4 mm
QW-403.8 change T Qualified 5 to 25.4 mm
QW-403.9 t pass > 13 mm None
QW-403.11 change P Qualified 1
QW-404 Filler metals
QW-404.4 change F Number 4
QW-404.5 change A Number 1
QW-404.6 change Diameter 3.2 mm
QW-404.7 change Diameter > (6 mm) None
QW-404.12 change Classification SFA 5.1 E7016
QW-404.30 change t 25.4 mm
QW-404.33 change Classification SFA 5.1 E7016
QW-405 Positions
QW-405.1 addition Position All
QW-405.3 change Vertical welding Upward
QW-406 Preheat
QW-406.1 Decrease > 55 deg. C Min. 10 deg.C
QW-406.2 change Preheat maintenance None
QW-406.3 Increase > 55 deg. C Max. 250 deg. C
QW-407 PWHT
QW-407.1 change PWHT None
QW-407.2 change PWHT (T & T range) None
QW-409 Electrical characteristics
QW-409.1 increase Heat input [note]
QW-409.4 change Current and Polarity DC EP
QW-409.8 change I & E range [note]
QW-410 Technique
QW-410.1 change String/weave string / weave
QW-410.5 change Method cleaning grinding, wire brushing
QW-410.6 change Method back gouge Grinding / Back gouging
QW-410.9 change Multi to single pass/ side Multi-passes
QW-410.25 change Manual or automatic Manual
QW-410.26 Addition/Deletion Peening None
QW-410.64 Use of thermal processes None

NOTE

  • QW-402.4: in case of preparation a new WPS from the combined PQR of GTAW + SMAW, the backing is stated “weld metal”.
  • QW-402.5 & QW-408.5: see definitions in QG-109.2.
  • QW-404.33 Carefully check in project specification, if any limitation manufacturer’s trade name.
  • QW-409.1 & QW-409.8: Heat input values and welding parameters follow project specifications.
  • Recommend base metal selection here.
  • Filler metal suggestion for welding procedures.

Free download template here.

P-No. 1 Gr-No. 1 to P-No. 1 Gr-No. 2 (1x2)

Other welding variables may preset the same above parameters and changing as below:

  • Material ASTM A516 Grade 60 to ASTM A516 Grade 70
  • P-Number 1 and Gr-Number 1 to P-Number 1 and Gr-Number 2
  • Thickness 12.7 mm.
  • Joint design: Groove, included angle 60 deg.
  • Position: 1G
  • Welding process: SMAW deposit 12.7 mm, manual, with backing

Welding Variables

Paragraph Variables SMAW
QW-402 Joints
QW-402.4 delettion Backing With backing
QW-403 Base Metals
QW-403.5 change Group Number Any Gr. 1 to any Gr. 2
QW-404 Filler metals
QW-404.12 change Classification SFA 5.1 E7016
QW-404.33 change Classification SFA 5.1 E7016
QW-410 Technique
QW-410.6 change Method back gouge Grinding / Back gouging

P-1 Gr.-2 to P-1 Gr.-2

Other welding variables may preset the same above parameters and changing as below:

  • Material: ASTM A516 Grade 70 to ASTM A516 Grade 70
  • P-Number 1 and Gr-Number 2
  • Thickness 12.7 mm
  • Joint design: Groove, included angle 60 deg.
  • Position: 1G.
  • Welding process: SMAW deposit 12.7 mm, manual, with backing

Welding Variables

Paragraph Variables SMAW
QW-402 Joints
QW-402.4 delettion Backing With backing
QW-403 Base Metals
QW-403.5 change Group Number Any Gr. 2 to any Gr. 2
QW-404 Filler metals
QW-404.12 change Classification SFA 5.1 E7016/18
QW-404.33 change Classification SFA 5.1 E7016/18
QW-410 Technique
QW-410.6 change Method back gouge Grinding / Back gouging

P-1 Gr.-1 (LTCS)

Other welding variables may preset the same above parameters and changing as below:

  • Material: ASTM A333 Grade 6 to ASTM A333 Grade 6
  • P-Number 1 and Gr-Number 1
  • Thickness 12.7 mm
  • Joint design: Groove, included angle 60 deg.
  • Position: 6G.
  • Welding process: SMAW deposit 12.7 mm, manual, with backing

Welding Variables

Paragraph Variables SMAW
QW-402 Joints
QW-402.4 delettion Backing With backing
QW-403 Base Metals
QW-403.5 change Group Number Any Gr. 1 to any Gr. 1
QW-404 Filler metals
QW-404.12 change Classification SFA 5.1 E7018-1
QW-404.33 change Classification SFA 5.1 E7018-1
QW-410 Technique
QW-410.6 change Method back gouge Grinding / Back gouging

NOTE:

QW-403.5; QW-403.6; QW-404.7; QW-404.12; QW-406.3; QW-407.2; QW-409.1; QW-409.4; QW-410.9 became essential variables.


paypal Thank you and Coffee :coffee:

WPS for P-No. 8

P-8 Gr.-1 to P-8 Gr.-1 (TP304)

  • Material: ASTM A240 TP304/304L
  • P-Number 8 and Gr-Number 1
  • Plate thickness 12.7 mm
  • Joint design: Groove, included angle 60 deg.
  • Position: 1G
  • Welding process: SMAW deposit 12.7 mm, manual, with backing.

General

Description of WPS here.

Welding Variables

Paragraph Variables SMAW
QW-402 Joints
QW-402.1 change Groove design Groove
QW-402.4 delettion Backing With/Without backing
QW-402.10 change Root spacing 3.0 - 4.0 mm
QW-402.11 deletion/addition Retainers None
QW-403 Base Metals
QW-403.5 change Group Number Any Gr. 1 to any Gr. 1
QW-403.6 T limits toughness 12.7 to 25.4 mm
QW-403.8 change T Qualified 5 to 25.4 mm
QW-403.9 t pass > 13 mm None
QW-403.11 change P Qualified 8
QW-404 Filler metals
QW-404.4 change F Number 5
QW-404.5 change A Number 8
QW-404.6 change Diameter 3.2 mm
QW-404.7 change Diameter > (6 mm) None
QW-404.12 change Classification SFA 5.4 E308L-15
QW-404.30 change t 25.4 mm
QW-404.33 change Classification SFA 5.4 E308L-15
QW-405 Positions
QW-405.1 addition Position All
QW-405.3 change Vertical welding Upward
QW-406 Preheat
QW-406.1 Decrease > 55 deg. C Min. 10 deg.C
QW-406.2 change Preheat maintenance None
QW-406.3 Increase > 55 deg. C Max. 150 deg. C
QW-407 PWHT
QW-407.1 change PWHT None
QW-407.2 change PWHT (T & T range) None
QW-409 Electrical characteristics
QW-409.1 increase Heat input [note]
QW-409.4 change Current and Polarity DC EP
QW-409.8 change I & E range [note]
QW-410 Technique
QW-410.1 change String/weave string / weave
QW-410.5 change Method cleaning grinding, wire brushing
QW-410.6 change Method back gouge Grinding
QW-410.9 change Multi to single pass/ side Multi-passes
QW-410.25 change Manual or automatic Manual
QW-410.26 Addition/Deletion Peening None
QW-410.64 Use of thermal processes None

NOTE

  • QW-402.4: in case of preparation a new WPS from the combined PQR of GTAW + SMAW, the backing is stated “weld metal”.
  • QW-402.5 & QW-408.5: see definitions in QG-109.2.
  • QW-404.33 Carefully check in project specification, if any limitation manufacturer’s trade name.
  • QW-409.1 & QW-409.8: Heat input values and welding parameters follow project specifications.
  • Recommend base metal selection here.
  • Filler metal suggestion for welding procedures.

Free download template here.

P-8 Gr.-1 (Type 316/316L)

Other welding variables may preset the same above parameters and changing as below:

  • Material: ASTM A240 TP316/316L
  • P-Number 8 and Gr-Number 1
  • Plate thickness 12.7 mm
  • Joint design: Groove, included angle 60 deg.
  • Position: 1G
  • Welding process: SMAW deposit 12.7 mm, manual, with backing.

Welding Variables

Paragraph Variables SMAW
QW-404 Filler metals
QW-404.12 change Classification SFA 5.4 E316L-15
QW-404.33 change Classification SFA 5.4 E316L-15

P-No. 8 Gr-No. 1 (TP304/304L to TP316/316L)

Other welding variables may preset the same above parameters and changing as below:

  • Material: ASTM A240 TP316/316L to TP304/304L
  • P-Number 8 and Gr-Number 1
  • Plate thickness 12.7 mm
  • Joint design: Groove, included angle 60 deg.
  • Position: 1G
  • Welding process: SMAW deposit 12.7 mm, manual, with backing.

Welding Variables

Paragraph Variables SMAW
QW-404 Filler metals
QW-404.12 change Classification SFA 5.4 E316L-15
QW-404.33 change Classification SFA 5.4 E316L-15

WPS for P-No. 1 to P-No. 8

P-No. 1 Gr-No. 1 to P-No. 8 Gr-No. 1

  • Material: API 5L Grade X52 to ASTM A240 TP316/316L
  • P-Number 1 and Gr-Number 1 to P-Number 8 and Gr-Number 1
  • Plate thickness 12.7 mm
  • Joint design: Groove, included angle 60 deg.
  • Position: 1G
  • Welding process: SMAW deposit 12.7 mm, manual, with backing.

General

Description of WPS here.

Welding Variables

Paragraph Variables SMAW
QW-402 Joints
QW-402.1 change Groove design Groove
QW-402.4 delettion Backing With/Without backing
QW-402.10 change Root spacing 3.0 - 4.0 mm
QW-402.11 deletion/addition Retainers None
QW-403 Base Metals
QW-403.5 change Group Number Any Gr. 1 to any Gr. 1
QW-403.6 T limits toughness 12.7 to 25.4 mm
QW-403.8 change T Qualified 5 to 25.4 mm
QW-403.9 t pass > 13 mm None
QW-403.11 change P Qualified Any P-No. 1 to any P-No. 8
QW-404 Filler metals
QW-404.4 change F Number 5
QW-404.5 change A Number 8
QW-404.6 change Diameter 3.2 mm
QW-404.7 change Diameter > (6 mm) None
QW-404.12 change Classification SFA 5.4 E309L-15
QW-404.30 change t 25.4 mm
QW-404.33 change Classification SFA 5.4 E309L-15
QW-405 Positions
QW-405.1 addition Position All
QW-405.3 change Vertical welding Upward
QW-406 Preheat
QW-406.1 Decrease > 55 deg. C Min. 10 deg.C
QW-406.2 change Preheat maintenance None
QW-406.3 Increase > 55 deg. C Max. 150 deg. C
QW-407 PWHT
QW-407.1 change PWHT None
QW-407.2 change PWHT (T & T range) None
QW-409 Electrical characteristics
QW-409.1 increase Heat input [note]
QW-409.4 change Current and Polarity DC EP
QW-409.8 change I & E range [note]
QW-410 Technique
QW-410.1 change String/weave string / weave
QW-410.5 change Method cleaning grinding, wire brushing
QW-410.6 change Method back gouge Grinding
QW-410.9 change Multi to single pass/ side Multi-passes
QW-410.25 change Manual or automatic Manual
QW-410.26 Addition/Deletion Peening None
QW-410.64 Use of thermal processes None

NOTE

  • QW-402.4: in case of preparation a new WPS from the combined PQR of GTAW + SMAW, the backing is stated “weld metal”.
  • QW-402.5 & QW-408.5: see definitions in QG-109.2.
  • QW-404.33 Carefully check in project specification, if any limitation manufacturer’s trade name.
  • QW-409.1 & QW-409.8: Heat input values and welding parameters follow project specifications.
  • Recommend base metal selection here.
  • Filler metal suggestion for welding procedures.

Free download template here.


paypal Thank you and Coffee :coffee:


P-1 Gr.-1 to P-8 Gr-1

  • Material: API 5L Grade X52 to ASTM A240 TP316/316L
  • P-Number 1 and Gr-Number 1 to P-Number 8 and Gr-Number 1
  • Plate thickness 12.7 mm
  • Joint design: Groove, included angle 60 deg.
  • Position: 1G
  • Welding process: SMAW deposit 12.7 mm, manual, with backing.

General

Description of WPS here.

Welding Variables

Paragraph Variables SMAW
QW-404 Filler metals
QW-404.12 change Classification SFA 5.4 E309L-15
QW-404.33 change Classification SFA 5.4 E309L-15

< Updating >


paypal Thank you and buy me a Coffee :coffee:


7 Likes

Test sample plate also qualified for all positions?

if all variables are unchanged and without impact test.
Qualified on plate shall also qualify for all positions.

Wow, clear my concern the WPS.
Keep up.

1 Like

Hello, topic had add table of content at right column.

2 Likes

Dear bien,
How can a coupon tested in 1G position qualified for all position?
1G PQR does not qualify for all positions as per QW-405.2.
When impact testing is required

In 2019 code book that portion is deleted? So now qualification on any positions/progression qualifies all progression?

Yes, QW-405.2 limits some welding processes - Supplementary essential QW-405.2 welding positions deleted in ASME IX 2019