AWS D1.1 2020 edition added 2 clauses - Normative References &Terms and Definitions.

MAIN CLAUSES

  • Clause 5: Pre-qualification of WPSs.
  • Clause 6: Qualification of WPSs.
  • Clause 10: Tubular Structure.

QUALIFICATION

Description Clause Remarks
PQR essential variable Table 6.5
PQR sup. essential variable Table 6.7
WPS qualification
- Position for plate Table 6.1
- Thickness for plate Table 6.2
- Position for tubular Table 10.8
- Thickness for tubular Table 10.9

Note: Table 6.7 are in addition the requirement of Table 6.5, see C-6.8.

To complete the WPS, we have a highlight in pWPS notes to minimize test coupon and reduce number of procedure.

  • Recommend the test coupon DN200x12.7 mm and DN80x5.5mm, see Table 10.9.
  • CVN requirement for welding procedure, above test coupons also complied with Table 6.7 line 2(a).
  • Recommend qualify a single process in a test coupon, instead of multiple process in a test coupon, see Table 6.5 line 34.

WELDING PROCEDURE SPECIFICATION

DESCIPTION OF WPS

JOINT DETAIL

I recommend to bring all essential variables in Table 6.5 and Table 6.7 to the WPS.

Refer to Table 6.5 for SMAW
Line #31: a change in groove type …
Line #32: a change in the type of groove to a square groove and vice versa.
Line #34: The omission, but not inclusion, of backing or back-gouging.

—WPS—

  • Groove type: Single V- or double V- Butt Joint or Fillet Joint.
  • Groove angle: as recommended in Figure 5.1 or 5.2.
  • Root opening: as recommended in Figure 5.1 or 5.2.
  • Root face: as recommended in Figure 5.1 or 5.2.
  • Back gouging and method: grinding or arc gouging.

POSITIONS

Refer to Table 6.5 for SMAW
Line #27: a change in position not qualified by Table 6.1 or 6.10 > See Table 6.1 for nontubular or Table 10.8 for tubular
Line #30: vertical welding > any changing from uphill to downhill and vice versa.

Refer to Table 6.7 for SMAW
Line #11: in the vertical position > change from stringer to weave bead.

BASE METAL

Approved base metal Spec / Grade or Type / AWS Grouping find in the Table 5.3 or AWS B2.1.

Refer to Table 6.5 for SMAW
Line #29: a change in base metal or combination of base metals not listed on the PQR or qualified by Table 6.8.

Refer to Table 6.7 for SMAW
Line #1: a change in group number.
Line #2(a): Min. thickness qualified…

—WPS—

  • PQR grouping the approved material qualification find in the Table 6.8.
  • Backing material: make sure material the same grouping number.
  • CJP groove welds thickness qualified: find in the Table 6.2 (Non-tubular) or Table 10.9 (Tubular).
  • CJP groove welds w/CVN thickness qualified: find in the Table 6.7 line #2 and Table 6.2 (Non-tubular) or Table 10.9 (Tubular).
  • CJP WPS shall qualify PJP Groove weld, see Clause 6.12.1.
  • Backing, refer to Clause 7.9.

FILLER METAL

Refer to Table 6.5 for SMAW
Line #1: Increase in filler metal classification strength.
Line #2: Change from low-hydrogen to non-low hydrogen SMAW electrode.
Line #4: Change to an electrode or flux electrode classification not covered in AWS A5.1 or A5.5
Line #10: Change in nominal filler metal diameter by increased 0.8 mm.

Any changes in essential variables, PQR required qualification.

—WPS—

  • AWS classification: type of electrode used for qualification, such AWS A5.1 E7108-1 or AWS A5.5 E11018M.
  • Diameter: detail max. diameter of electrode and additional allowance in Line #10 above such max. 4.0 mm.

PRE-HEAT

Refer to Table 6.5 for SMAW
Line #35: Decrease from preheat temperature by 15 deg. C.
Line #36: Decrease from inter-pass temperature by 15 deg. C.
Refer to Table 6.7 for SMAW
Line #8: An increase of more than 100°F [56°C] in the maximum preheat or interpass temperature qualified

—WPS—

  • Min. preheat temperature: refer to PQR recorded and Table 5.3, Table 6.9.
  • Max. inter-pass temperature: refer to PQR recorded and Table 6.9.

PWHT

Refer to Table 6.5 for SMAW
Line #37: addition or deletion of PWHT.
Refer to Table 6.7 for SMAW
Line #9: a change in the PWHT time and range …

—WPS—

  • PWHT temperature: see Clause 7.8.

GAS

This section is not applicable for SMAW process.

TECHNIQUE

Refer to Table 6.7 for SMAW
Line #11: In the vertical position, a change from stringer to weave.
Line #12: A change from multi-pass per side to single pass per side

ELECTRICAL CHARACTERISTICS

Refer to Table 6.5 for SMAW
Line #12: A change in the amperage for each diameter used by manufacturer.
Line #13: A change in type of current (ac or dc) or polarity (electrode positive or negative for dc current).
Refer to Table 6.7 for SMAW
Line #10: An increase in heat input or volume of weld metal deposited per unit length of weld, over that qualified, …

—WPS—
Welding parameters should minimum follow:

  • Layer / pass of process:
  • Filler metal: class. and diameter
  • Current and Polarity:
  • Amperage and Voltage:
  • Travel Speed:
  • Heat input per length:
  • Other:

Procedure Qualification Records

Testing Requirement

Type of CJP weld qualification tests are required in Clause 6.5

Below table is a sample of testing required.

# Type of tests Clause/Figures reference Acceptance criteria Result Remarks
1 Visual inspection 6.10.1 6.10.1 - -
2 RT 6.10.2.1 6.10.2.2 - -
3 Side bends 6.10.3.1 / Fig. 6.9 6.10.3.3 - -
4 Tensile test 6.10.3.1 / Fig. 6.10 6.10.3.5 - -
5 Macro-etch 6.10.4 6.10.4.1 - -
6 CVN tests 6 Part D/ Fig. 6.28 6.30 and Table 6.14 - -
  • CVN evaluation, see C-6.27.

OTHER

  • Welder name, number shall be recorded in the PQR.
  • Laboratory body shall be recorded in the PQR. I recommend a recognized body to conduct the testing.

Download WPS forms and request for services.


 

Leave a comment


This site uses Akismet to reduce spam. Learn how your comment data is processed.


FIND YOUR TOOL ON AMAZON

wic_amazon
WIC-2560x512 Community

Services

Contact Us

Following Us

Disclaimer: Weldinginspections.net is based on information from multiple sources and our experience with welding and inspection scopes. It is not a replacement for manufacturers directions and is only to provide reminders for inspector.

© 2019 - 2021 weldinginspections.net | All rights reserved | Privacy Policy